In coatings, aluminum powder serves two primary functions: creating a metallic appearance and providing a shielding effect. Aluminum exists as flake-like particles with sub-micron thickness and a high aspect ratio; a metallic look is achieved only when these flakes are aligned parallel to one another. The challenge in dispersing aluminum powder lies not in breaking up agglomerates, but in ensuring that the flakes remain intact and preventing any reaction between the aluminum and water. In fact, when issues arise with aluminum-pigmented coatings, seven or eight times out of ten, the problem stems from hydrogen evolution or poor flake orientation—not from a lack of fineness. (The specific model mentioned is provided solely to illustrate the structural concept.)

 

I. Fundamental Principles: The Two Fatal Flaws of Aluminum Pigments

The first fatal flaw is water. Aluminum is a highly reactive metal that releases hydrogen upon contact with water—a chemical reaction familiar to everyone. This is the root cause of issues in waterborne aluminum-pigmented coatings, such as container swelling, blistering, or even deformation of the drums. Introducing bare aluminum pigment into a waterborne system—without proper encapsulation—will inevitably lead to problems. Common encapsulation strategies include coating the particles with silicon, silicon dioxide, or acrylic polymers; the integrity of this coating layer determines the product's shelf life.

 

The second fatal flaw is shear. Aluminum flakes are sub-micron in thickness with an aspect ratio (diameter-to-thickness) of several dozen; under high-shear conditions, these flakes can fracture or develop curled edges. Once fractured, the reflection shifts from specular (mirror-like) to diffuse, causing the metallic luster to turn into a dull gray, while also compromising hiding power. Therefore, the dispersion process for aluminum pigments requires a delicate balance: breaking up agglomerates without damaging the flakes themselves. High-energy equipment, such as bead mills (sand mills), is generally unsuitable for this purpose.

 

The mechanisms for "leafing" and "non-leafing" aluminum pigments are entirely different. Leafing pigments feature a surface layer of stearic acid-based lubricant, which results in low surface energy. As the paint film dries, surface tension gradients cause the flakes to rise to the surface, forming a continuous, mirror-like layer. For leafing pigments, the key requirement for a dispersant is that it must not interfere—a dispersant with excessive polarity can strip away the lubricant layer, preventing the flakes from rising. Non-leafing pigments, by contrast, rely on resin encapsulation and specific orientation of the flakes; here, the dispersant must ensure stability, often working in tandem with wax pastes or orientation additives to ensure the flakes remain aligned parallel to the substrate.

 

Another characteristic of aluminum pigments is that their hiding power depends on the "number of overlapping layers." At a constant dosage, the more intact the flakes are and the more parallel their alignment, the greater the hiding power. If the dispersion process is poorly executed, one might be tempted to compensate for insufficient hiding power by adding more pigment—but this only increases costs while further degrading the metallic appearance.

 

II. The Complete Selection Process

Defining Basic Boundary Conditions

Powder Characterization: Determine whether the powder is of the "leafing" or "non-leafing" type; assess particle size and aspect ratio (diameter-to-thickness ratio); identify the presence and type of any surface coating; and determine the solids content (aluminum-silver pastes are typically supplied in a solvent or aqueous carrier). For waterborne systems, only coated pigments are suitable for long-term storage; using uncoated powders in such systems is essentially inviting trouble.

System Definition: Identify the binder system—waterborne (acrylic, polyurethane, or alkyd), solvent-borne (thermoplastic acrylic, alkyd-amino, or two-component polyurethane), UV-curable (monomer-diluted; note that aluminum pigments can block UV light), or resin-free aluminum pastes.

 

Application Method: Consider whether the coating will be applied via spraying, roller coating, or dipping. Spraying involves low shear, whereas roller coating involves high shear; for the latter, select grades with more robust, structurally sound flakes.

Performance Parameters: Evaluate requirements for metallic effect, "flop" (angle-dependent color variation), hiding power, water and alkali resistance, hydrogen evolution during storage, and adhesion. For automotive coatings, weather resistance and acid-rain resistance must also be considered.

Key Note: In waterborne aluminum pigment systems, conduct a hydrogen evolution test before selecting a dispersant. If gas generation exceeds limits within seven days, changing the dispersant is futile—the issue lies with the coating layer on the pigment. Getting this sequence wrong renders all subsequent preliminary testing meaningless.

 

Type Selection

Water-based systems: Opt for polymeric dispersants with low polarity and a low acid value. These utilize amide groups and weak carboxylic acid groups for anchoring, avoiding the use of strong acid groups that could erode the coating layer on the aluminum flakes. Products such as HR-4044 and HR-4065 (examples provided solely to illustrate molecular structure types) feature multiple anchoring sites and offer a milder compatibility with coated aluminum pigments, making them suitable for water-based industrial coatings and water-based metallic basecoats. If the formulation also contains colored pigments, a general-purpose anchoring dispersant may be added; however, ensure the total concentration of dispersant is not too high, as free (unadsorbed) dispersant components can accelerate hydrogen evolution in water-based aluminum pigment systems.

 

Solvent-based systems: The primary challenges in solvent-based aluminum pigment coatings are achieving proper flake orientation and ensuring storage stability. For leafing-type aluminum pigments, use dispersants with low polarity—or, in some cases, omit solid dispersants entirely, relying instead on wetting agents and solvent balance. For non-leafing-type pigments, polymeric dispersants containing aromatic groups are preferred. Products such as HR-4021 and HR-4037B (examples provided solely to illustrate molecular structure types) exhibit good compatibility in esters and aromatic hydrocarbons, facilitating the stable dispersion of non-leafing aluminum pigments. To enhance flake orientation, a controlled flocculation structure can be introduced; for instance, HR-8030 (an example provided solely to illustrate molecular structure types) allows the aluminum flakes to form weak flocs that move in unison, which facilitates their parallel alignment during the drying process.

 

UV Systems: The primary challenge with UV-curable metallic coatings is that aluminum flakes block UV light, leading to insufficient curing of the underlying layers. Furthermore, high monomer shrinkage can cause the flakes to shift out of alignment. It is best to select solvent-free, low-viscosity formulations and incorporate orientation-promoting waxes. The dosage of dispersants should be kept to the absolute minimum; an excess will retard the curing process and compromise adhesion.

 

Resin-free Aluminum Pastes: These products are often prepared in-house by aluminum pigment manufacturers or color-matching centers for use across various coating systems. The key is to avoid products containing silicon or fluorine, as well as those with high acid values—specifically those with strong acidic functional groups—which can destroy both the protective coating (encapsulation) on the flakes and the lubricating layer responsible for their "leafing" (floating) orientation.

 

❌ Products to Avoid: Strongly acidic phosphate esters should be used with extreme caution in waterborne aluminum pigment systems; their acidity can erode the protective encapsulation and trigger hydrogen evolution. Small-molecule anionic surfactants, while providing rapid wetting, fail to stabilize the flakes and can easily strip away the lubricating layer required for proper orientation. Similarly, using silicon-based additives as dispersants is not recommended; silicon lowers surface energy, which disrupts the desired orientation of "leafing" (floating) aluminum pigments.

 

3. Small-Scale Evaluation Process

Begin with screening for encapsulation stability and hydrogen evolution. Incorporate the aluminum paste into the aqueous system at the target ratio, seal the container, and let it stand for seven days. Measure the volume of gas generated and the internal pressure; proceed to dispersant screening only if the results are satisfactory.

 

Use low-energy dispersion methods, such as low-speed stirring or the lower-energy range of high-speed dispersion. Bead milling and prolonged high-shear (high-tip-speed) processing are strictly prohibited, as aluminum flakes cannot withstand such mechanical stress.

 

Test dispersants using a concentration gradient of 1% to 5% (based on the weight of the aluminum paste or the powder content). For "leafing" (floating) systems, use a narrower range—often comparing only a "zero-addition" control against a "low-addition" sample.

 

Evaluate initial fineness (using a fineness gauge, taking care to avoid excessive pressure), hiding power, flop (color variation with viewing angle), and gloss at 20° and 60°. For metallic coatings, angular gloss is critical; relying solely on 60° gloss is insufficient.

 

Conduct stability testing, including storage at 50°C for seven days and at room temperature for 30 days. Monitor for gas evolution, sedimentation, and changes in metallic appearance. For aqueous systems, also perform freeze-thaw stability testing.

 

Carry out downstream validation: assess flake orientation and flop on sprayed test panels; check for flake integrity in roller-coated applications; and evaluate adhesion and recoatability when applied in conjunction with a topcoat.

 

III. Common Issues, Causes, and Solutions

Can swelling or gas pressure upon opening: This occurs when the protective coating on the aluminum flakes is incomplete, allowing direct contact between the aluminum and water, or when the acid value of the dispersant is too high, eroding the coating. Solutions include using aluminum paste with a more intact coating, lowering the acid value of the dispersant, maintaining a neutral-to-slightly-alkaline pH, and controlling storage temperatures.

 

Dull metallic appearance (grayish) and insufficient hiding power: This happens when aluminum flakes are sheared, fractured, or curled, causing light reflection to shift from specular (mirror-like) to diffuse. Solutions include reducing shear forces, eliminating sand-milling processes, switching to more shear-resistant flake types, and minimizing the dispersant dosage to the critical threshold.

 

Poor "flop" (insufficient color variation with viewing angle), appearing dark when viewed head-on and bright from the side: This is caused by poor orientation of the aluminum flakes, where they fail to align in parallel. Solutions include adding orientation waxes or introducing a controlled flocculation structure, and adjusting the solvent evaporation gradient to ensure the flakes remain fixed in place during the drying window.

 

"Leafing" aluminum pigments failing to rise to the surface, resulting in a dark paint film: This occurs when the dispersant is too polar, stripping away the stearic acid lubricating layer from the flakes. Solutions include switching to a less polar dispersant, reducing the dispersant dosage, and verifying whether the solvent system is dissolving the lubricating layer.

 

Aluminum pigment settling and forming a "hard cake" during storage, with the metallic effect failing to recover after stirring: This happens when the flakes become compacted and adhered to one another within the container. Solutions include reinforcing the thixotropic structure or employing controlled flocculation to ensure the flakes settle as a loose, uniform mass—preventing the formation of a dense, hard cake—and avoiding the use of high-shear agitation.

 

IV. Key Points for Selection

The primary principle for dispersing aluminum pigments is "protecting the flakes," while the secondary principle is "controlling water." In waterborne systems, the focus must first be on encapsulation and the prevention of hydrogen evolution before addressing the choice of dispersant. In solvent-borne systems, one must distinguish between leafing and non-leafing grades: leafing pigments require a low-polarity environment with minimal interference, whereas non-leafing pigments require stabilization and proper orientation. Dispersion equipment should always be of the low-shear type; bead milling is not an appropriate option. The quality of the dispersion should be evaluated based on color travel (flop/goniochromatism) and hiding power, rather than on particle fineness.

 

FAQ

1. Why shouldn't aluminum pigments be processed via bead milling? Aluminum flakes are sub-micron thick with a high aspect ratio; bead milling causes them to fracture and their edges to curl. This transforms specular reflection into diffuse reflection, resulting in a loss of both metallic luster and hiding power.

2. What causes container swelling in waterborne aluminum-pigment paints? It is due to the reaction between aluminum and water, which releases hydrogen gas. First, verify the integrity of the pigment’s protective coating; then, check the acid value of the dispersant and the pH of the system. Simply changing the dispersant is unlikely to solve the problem.

3. Can the same dispersant be used for both leafing and non-leafing aluminum pigments? It is not recommended. Leafing pigments require a low-polarity environment with minimal interference; high-polarity substances can strip away the lubricating layer. Non-leafing pigments, by contrast, require stable dispersion combined with proper orientation.

4. What should be done if the "flop" (color shift at different viewing angles) is not distinct? This usually indicates poor flake orientation. Consider adding orientation waxes or introducing a controlled flocculation structure. Additionally, adjust the solvent evaporation gradient to ensure the flakes remain fixed in place during the drying window.

5. Is insufficient hiding power in aluminum-pigment paints a result of particle fineness? Usually, it is caused by fractured flakes or a lack of parallel alignment. Investigate the shear history and flake orientation; do not attempt to compensate simply by adding more pigment.

6. What precautions are necessary for UV-curable metallic coatings? Aluminum pigments block UV light, so the curing of the underlying layers must be carefully verified. Select a solvent-free, low-amine dispersant, and keep the dosage at the absolute minimum required for stability.

7. What are the principles for selecting a dispersant for resin-free aluminum pastes? Avoid products containing strong acids, silicones, or fluorine. The dispersant should protect the pigment’s protective coating and any leafing-promoting lubricating layers, while prioritizing compatibility across different systems.